32.1 Concrete Testing: Slump & Strength
Key Takeaways
The ASTM C143 cone is 4 inches across the top, 8 inches across the base and 12 inches tall. Fill three layers of about equal volume, rod each 25 times and lift straight up in 5 ± 2 seconds.
Prescriptive foundation-wall concrete in removable forms ordinarily has a 6-inch maximum slump, with a separate approval exception. In stay-in-place forms slump must exceed 6 inches, and the default is internal vibration unless an approved qualifying self-consolidating mixture is used.
Under ACI 318, every average of three consecutive strength tests must meet the specified strength. Each test must also meet its individual floor, which is specified strength minus 500 psi for mixes specified at 5,000 psi or less.
A 7-day result of 2,250 psi is 75% of a 3,000 psi specified strength. Use it as early information and evaluate acceptance at the specified testing age.
When the ACI 318 low-strength investigation uses ASTM C42 cores, the area passes the structural adequacy criteria if the average of three cores is at least 85% of specified strength and each core is at least 75%.
Fresh tests describe the concrete delivered. Strength tests describe the hardened material at the specified age. Start with the approved mix identification and exposure requirements. Under MRC Table R402.2, the severe-weathering baseline for exposed exterior foundation walls and other exposed vertical work is 3,000 psi at 28 days. Unexposed foundation concrete has a 2,500 psi baseline. Check the seismic, air and other applicable conditions before accepting the delivery.
Sampling before testing
For ready mix from a revolving-drum truck, ASTM C172 uses portions at two or more regularly spaced intervals in the middle of discharge, after the required batch adjustments. Combine the portions within 15 minutes of starting collection. Start slump, air and temperature tests within 5 minutes of the final portion and start molding strength specimens within 15 minutes of making the composite sample. For ACI 318 acceptance, sample at delivery. If the construction documents specify a separate test at pump discharge or point of placement, use the specified sampling protocol and criteria there.
The slump test (ASTM C143)
The slump test measures consistency, the vertical change in height after the mold is removed. Compare the result with the specified slump and applicable tolerance. The test result alone establishes neither the mixture proportions nor the compressive strength.
- Set up. Dampen and hold the 4-inch top, 8-inch base, 12-inch tall cone on a level, rigid, moist, nonabsorbent surface. Use the standard rounded 5/8-inch tamping rod.
- Fill three layers of equal volume. The first reaches about 2-5/8 inches above the base, the second about 6-1/8 inches above the base, and the third reaches the top. The cone tapers, so the layers have different heights.
- Rod 25 times per layer. Rod the first through its depth. Rod the next two through their layers and about 1 inch into the layer below. Keep the top layer above the rim while rodding.
- Strike off and clean the base. Remove any spill that would interfere with the slump.
- Lift vertically in 5 ± 2 seconds. Avoid twisting and lateral movement. Work steadily and finish filling through mold removal within 2-1/2 minutes.
- Measure immediately. Report the vertical difference from the mold height to the displaced original center of the specimen’s top surface, to the nearest 1/4 inch.
If part of the specimen shears away, disregard that result and repeat on another portion of the sample. Two consecutive shear results indicate the mix may lack the plasticity or cohesion needed for the test. A collapse indicates that the usual vertical slump may lack significance. Check the governing procedure for the mix, such as the horizontal spread test under ASTM C1611 for self-consolidating concrete.
Reading the number
The same slump can come from different proportions. A water reducer can make a low-w/cm mix more fluid. An unmeasured water addition can make an otherwise similar mix more fluid and reduce its strength. Compare delivery results to the specified slump range and use independent strength tests.
| Concrete placement | Slump rule |
|---|---|
| Foundation walls, removable forms | Maximum 6 inches unless an approved segregation-resistant mix meets the manufacturer’s recommendations |
| Foundation walls, stay-in-place forms (ICF) | Greater than 6 inches, measured under ASTM C143 |
Under R404.1.3.3.5, stay-in-place foundation forms require internal vibration unless an approved self-consolidating mix with at least 8 inches of slump is specifically designed for placement without it. For flatwork, use the project slump and follow the approved placement procedure.
A permitted jobsite adjustment must stay within the specified slump and water-to-cementitious materials ratio. Check the ticket and producer’s allowance, measure and record the addition, and remix and retest as required. Extra unaccounted-for water raises the ratio and can reduce strength and durability.
Cylinders: ASTM C31 and ASTM C39
Keep the specimen counts for a strength test separate from the number of separate batch samples. Under ACI 318-14, referenced by the 2015 MRC where ACI 318 applies, one acceptance test is the average of at least two 6 × 12-inch cylinders or at least three 4 × 8-inch cylinders from the same sample at the specified age. ACI 318-19 retains those counts. ACI 318-25 permits at least two of either size. Use the adopted or specified edition and check the contract for any additional specimens.
Making and curing, ASTM C31. Use a cylinder diameter at least three times the nominal maximum coarse aggregate size. When rodding, place concrete in three layers for a 6 × 12-inch cylinder and two for a 4 × 8-inch cylinder, with 25 strokes per layer using the rod for that mold size. Tap the mold as specified and finish the top. Protect standard-cured specimens from moisture loss, disturbance and temperature extremes for the initial curing period of up to 48 hours. Maintain 60°F to 80°F for ordinary concrete or 68°F to 78°F when specified strength is at least 6,000 psi. Follow the standard for timing and protected transport. For final standard curing, maintain free water on the specimen surface at 73.5 ± 3.5°F under the laboratory procedure.
Testing, ASTM C39. Use compliant ground, capped or unbonded ends and load the centered specimen to failure in compression. Divide maximum load by the measured cross-sectional area. Report irregularities and the fracture pattern. Several fracture patterns can occur with acceptable tests, so use the specimen condition, test records and procedure when evaluating a suspect result.
Sampling frequency where ACI 318 governs. For each mix, satisfy all three minimums: once each placement day, once per 150 yd³ and once per 5,000 ft² of slab or wall surface. If this would produce fewer than five tests for a mix, sample at least five randomly selected batches or all batches if there are fewer than five. For a mix totaling less than 50 yd³, the building official may accept submitted evidence of satisfactory strength in place of tests. For form removal or loading, use field-cured specimens or another approved in-place strength method.
7-day versus 28-day strength
28 days is the usual acceptance age. Use the specified age when different. An early result at 7 days helps track strength development. The cementitious materials, temperature and curing affect its relationship to the acceptance-age result.
Worked example. Concrete specified at 3,000 psi at 28 days gives 2,250 psi at 7 days. The early result is 75% of specified strength. Compare it with the approved mixture’s early-age data and use the acceptance-age test for the acceptance decision.
Second example. Another batch of the same mix gives 1,800 psi at 7 days, or 60% of specified strength. That ratio alone cannot predict the later result. If it is low relative to comparable early-age records, check sampling and cylinder curing and review the delivery and adjustment records. Apply the specified age and criteria to decide acceptance.
Acceptance criteria under ACI 318
Strength results are accepted when both conditions hold:
- The average of any three consecutive strength tests equals or exceeds f-prime-c.
- No single test falls below f-prime-c minus 500 psi when f-prime-c is 5,000 psi or less. Above 5,000 psi the floor becomes 0.90 f-prime-c.
For a 3,000 psi specification, tests of 3,150, 2,700 and 3,150 psi average 3,000 psi. Each is above 2,500 psi, so that three-test window satisfies both limits. Keep checking each consecutive window. Each reported test is a specimen average from one sample.
The other field tests
| Test | Standard | What it tells you |
|---|---|---|
| Slump | ASTM C143 | Vertical slump, an index of consistency |
| Air content by pressure | ASTM C231 | Total fresh air for suitable, relatively dense aggregates |
| Air content by volume | ASTM C173 | Total fresh air, including mixes with lightweight or porous aggregate |
| Temperature | ASTM C1064 | Fresh concrete temperature at the sampling location |
| Density and yield | ASTM C138 | Mass per volume and calculated volume yielded by the batch |
Use the Michigan severe-weathering column of Table R402.2. The listed exposed vertical and flatwork applications generally use 5% to 7% total air. Read the footnotes for protected work freezing during construction and for the optional steel-troweled garage mix of at least 4,000 psi with at least 3% air. Air voids reduce freeze-thaw damage. Select the air test for the aggregate.
Check fresh concrete temperature against the placement specification and protection plan. Heat can accelerate set and slump loss. Premature freezing can permanently damage fresh concrete. Temperature, time and protection history also help interpret early test results.
To check yield, divide the total batch mass by its measured density. For example, 39,150 lb ÷ 145 lb/ft³ = 270 ft³ = 10 yd³. If the computed volume differs from the order, verify the batch mass and density measurement before diagnosing why.
When a test fails
A failed rolling-average criterion calls for steps to improve subsequent production. An individual test below its allowable floor or field-cured results indicating inadequate protection can require a structural investigation.
- Verify the evidence. Review sampling, specimen curing, handling, ends and test records. Keep all results and document technical reasons for questioning any result.
- Trace the concrete. Match the test to the installed area and review the ticket and changes to the batch. Report the issue to the parties responsible for the evaluation.
- Protect the structure. If low strength is likely and calculations indicate that structural adequacy is significantly reduced, have the responsible professional evaluate whether ASTM C42 cores are warranted. A later truck tests a different batch.
- Apply the core criteria where the ACI procedure is used. Take three cores for each individual strength test below the allowable floor. The area represented is structurally adequate under the core criteria when the average is at least 85% and every core is at least 75% of specified strength. For a 3,000 psi specification, those thresholds are 2,550 psi average and 2,250 psi per core.
- Resolve remaining doubts. Additional cores may be appropriate for erratic results. If adequacy remains in doubt, the responsible design professional and building official determine the applicable evaluation or corrective path.
Exam traps to expect
- Compare the slump with its specification, and use separate evidence for strength.
- Apply the removable- and stay-in-place-form provisions to their own assemblies.
- Keep the early-age break, acceptance-age test and in-place strength evaluation distinct.
- Apply both the rolling average and individual floor to strength tests, using specimen counts from the governing edition.
- Apply the core criteria to the area evaluated under the low-strength procedure.
A standard ASTM C143 slump cone has which dimensions?
4 inches across the top, 8 inches across the base, 12 inches tall
6 inches across the top, 12 inches across the base, 18 inches tall
4 inches across the top, 8 inches across the base, 6 inches tall
8 inches across the top, 12 inches across the base, 12 inches tall
Under the ACI 318 cylinder acceptance criteria, which pair of limits applies at the specified age for a 3,000 psi mix?
Every individual test must equal or exceed 3,000 psi
The average of any two consecutive tests must exceed 3,000 psi
No test may fall below 3,000 psi and each must be within 10 percent of the average
The average of any three consecutive tests is at least 3,000 psi and no single test is below 2,500 psi
A concrete mix specified at 3,000 psi at 28 days gives a 7-day strength test of 2,250 psi. What can this result establish?
The concrete has failed and cores must be drilled immediately
The early result is 75% of the specified strength, and acceptance is evaluated at the specified 28-day age
The concrete will reach exactly 2,250 psi at 28 days
The result is the final acceptance test and the concrete must be removed