33.3 Concrete Finishing

Key Takeaways

  • Complete initial leveling before bleeding. Wait until bleeding has ceased and the surface can support the operation before final floating, troweling or texturing.

  • Strike off, then level promptly with a bull float or darby. Time edging and tooling to suit the finish and joint method. Float after bleeding ceases, apply the selected finish and start curing promptly.

  • Use a nearly flat bull float to level the fresh concrete and embed coarse aggregate without sealing the surface prematurely.

  • ACI 305.1 hot-weather work uses the specified evaporation action level. Consider concrete and air temperatures, humidity and near-surface wind. Low-bleed mixtures may need protection below 0.2 lb/ft²/h.

  • ACI 306R-16 cold-weather guidance applies when the air will fall below 40°F during the protection period. For sections less than 12 inches thick, its recommended minimum concrete temperature as placed and maintained is 55°F.

Last updated: November 2026

Quick Answer: Strike off and level with a bull float or darby before bleed water appears. After bleeding ceases and the slab firms up, float and apply the specified final finish. Protect the surface from evaporation between operations and start curing as soon as the finish permits.

The Sequence and Why the Order Matters

Judge the timing from the condition of the concrete. The weather and mix can shift the window from one placement to the next.

OperationTiming cuePurpose
Strike-off (screeding)As concrete is deposited and consolidatedEstablish the surface elevation and remove excess
Bull float or darbyPromptly after strike-off, before bleed water appearsLevel peaks and hollows and embed coarse aggregate
Wait and protectUntil bleeding has ceased and the surface supports the next operationPrevent a closed surface over continuing bleed
Edge and tool jointsWhile concrete can hold the specified edge or groove, adjusting the sequence to the finishForm edges and locate contraction joints without tearing the surface
Float (hand or power)Once bleeding has ceased and the surface supports the toolLevel and compact the surface mortar
Final finishOnce it will hold the required texture or trowel passProduce the specified surface for the use and exposure
CurePromptly when the final surface can accept the selected methodKeep moisture available for hydration

MRC R506.1 generally sets a 3-1/2-inch minimum for concrete floors on ground. The finishing choice also depends on intended traffic, drainage, exposure and the mixture.

Screeding and Bull Floating

Screeding strikes concrete to grade using a straightedge, powered screed or another specified method. Place concrete near its final position and use the equipment appropriate to the slump and consolidation plan.

A bull float uses a long handle to reach across a slab. A darby is a hand tool for the same initial leveling operation on narrower work. Before bleeding:

  • level ridges and hollows from strike-off,
  • embed aggregate near the top of the fresh slab,
  • leave a uniform surface for later finishing.

Keep the float nearly flat. Excessive passes or a steep blade can close the surface too early and trap air and water below it.

The Bleed-Water Trap

As solids settle, bleed water can rise to the surface. A dry-looking crust can form while bleeding continues below it. A temporary cover on a small area can help determine whether bleeding is still occurring.

Wait before final finishing. The surface should have finished bleeding and be able to support the next operation. Working standing water into the surface weakens the paste. Closing a surface while water or air is still rising can trap it below the finish.

  • Dusting is a weak, powdery surface that wears away.
  • Crazing is a network of fine surface cracks associated with surface shrinkage.
  • Blistering or delamination can occur when a dense finish traps bleed water or air.
  • Scaling is surface loss that can be aggravated by weak surface paste, freeze-thaw exposure and deicers.

Keep added water and dry cement off the surface during finishing. Air fogging for evaporation control is a separate operation. Prevent water from collecting on the slab.

Floating, Troweling and Overworking

Floating compacts the mortar and brings a small amount of paste to the surface so the trowel can close the concrete. Hand floats are wood or magnesium; power floats use rotating pans. Float after bleed water has cleared, and keep the machine moving.

Troweling hardens and densifies the surface. Hand steel trowels start flat and are tilted progressively; power trowels do the same with blade pitch and machine weight. A burnished finish takes multiple passes at increasing pitch.

Select the finish for service conditions. Hard steel troweling of air-entrained concrete can trap air and water. A textured finish is typical outside and improves traction. A steel-troweled Michigan garage slab has separate strength and air provisions under R402.2 and still requires an approved mix and finishing plan.

Edging, Jointing and Brooming

Run an edger while the concrete takes the specified profile without tearing. Use the edge radius and tool required by the detail.

Tool a contraction joint while the concrete can form and hold the required groove. Restore the groove on a later pass if needed. For sawed joints, verify depth, timing and layout separately.

Broom the surface when it can hold the specified texture. For a walk, brooming across traffic commonly gives the wanted traction. Use a trial pass to check whether the bristles tear the paste or leave grooves that close up.

Stamped and Decorative Finishes

Stamped concrete is flatwork with a pattern pressed into it. The sequence is exacting:

  1. Choose the approved decorative system before placing. Integral color goes into the mix. A compatible dry-shake hardener goes on the fresh surface at the manufacturer’s specified stage.
  2. Strike off, level and manage bleed water. Follow the product’s release-agent and stamping window.
  3. Align the mats and stamp while the surface can hold the imprint. Protect edges and form or saw joints per the layout.
  4. Follow the system’s cure, residue removal, drying and sealer instructions. Some products act as a cure and seal. Check the slip-resistance requirements for the setting.

Confirm weather and surface condition before applying a sealer. Moisture or contamination can degrade film appearance or bond.

Hot, Windy Weather: The Evaporation Problem

In warm, dry or windy conditions, evaporation can outrun bleeding and lead to plastic shrinkage cracking before hardening. The risk also depends on how much the mixture bleeds.

ACI 305.1 uses 95°F at discharge as its specified default upper limit, subject to the applicable specification. Check the evaporation action level in the job documents. 0.2 lb/ft²/h (about 1 kg/m²/h) is a common specification threshold for protective action. Low-bleed mixtures can require protection at a lower estimate.

Plan evaporation controls before the concrete arrives:

  • Arrange shade or windbreaks and place at a cooler, calmer time when feasible.
  • Prepare dry absorptive surfaces as specified, with no standing water and without disrupting any required vapor retarder.
  • Use fogging or an approved evaporation retardant as appropriate. Avoid ponding, and follow the product instructions.
  • Arrange a suitable concrete temperature and working time with the producer. Apply the specified curing method promptly.

Worked Scenario: Driveway on an 85°F, Windy Day

A 20 × 24 ft driveway, 5 inches thick, is scheduled for 1 p.m. Assume 85°F air and concrete, 25% relative humidity, and 15 mph wind near the slab surface. Using the FHWA fit for the ACI evaporation nomograph gives about 0.32 lb/ft²/h (1.57 kg/m²/h). That estimate exceeds the example action level of 0.2 lb/ft²/h. Recheck with actual conditions at placement.

Adjusted plan:

  1. Move placement earlier or install shade and wind protection. Prepare the subgrade as specified.
  2. Confirm approved slump and concrete temperature with the producer. Follow the delivery procedure for an authorized adjustment.
  3. Strike off and bull float promptly. Protect against evaporation between operations and check whether the slab is still bleeding beneath a dry-looking surface.
  4. Float and broom when the surface is ready. Start the specified cure as soon as the finished texture can accept it.
  5. Under the example 24-to-36 multiplier, 5 inches gives 10 to 15 ft. A 2 × 2 layout across the 20 × 24 ft rectangle yields 10 × 12 ft panels. Use the approved joint geometry and start sawing while the surface holds an edge and before random cracking.

If the surface crusts before bleeding stops, check the slab and maintain evaporation controls. Starting a steel trowel on that crust can close it over water that is still rising.

Cold-Weather Finishing

ACI 306R-16 treats cold weather as air temperature that has fallen or is expected to fall below 40°F during the protection period. Use the applicable cold-weather plan:

  • Prepare a thawed bearing surface free of ice and snow.
  • Under ACI 306R-16, sections less than 12 inches thick have a recommended minimum of 55°F as placed and maintained. The larger section-size bands have lower recommended minimums. Use the project’s temperature and protection criteria.
  • Arrange any heat or approved accelerator in advance and keep insulated covers or an enclosure ready. Vent combustion heaters so exhaust does not reach fresh concrete. Carbon dioxide from exhaust can cause a weak, dusty surface.

Protect against a single early freeze until the concrete reaches about 500 psi. That threshold addresses one freeze. The curing period, protection against repeated cycling and strength for loading are separate decisions.

Defect-Cause Table

DefectPossible contributorControl
DustingSurface water worked in, or combustion exhaust at the surfaceKeep water off during finishing and vent heaters
CrazingDifferential drying and shrinkage at the surfaceAvoid excessive finishing and cure promptly
Blistering or delaminationA closed skin over rising air or waterConfirm bleeding has ceased and use the specified finishing procedure
ScalingWeak surface paste, inadequate air or freeze-thaw and deicer exposureUse the applicable mix, finish and cure
Plastic shrinkage cracksSurface evaporation that exceeds bleedingAssess conditions and maintain evaporation controls
Test Your Knowledge

A basement slab has been struck off and bull floated. Bleed water has risen. What should the crew do before applying the specified floated and troweled finish?

A

Steel-trowel now to keep the surface from drying.

B

Wait until bleeding ceases and the surface can support the finishing operation.

C

Sprinkle dry cement over the surface to absorb the water.

D

Mist the surface and trowel while water is still standing.

Test Your Knowledge

For a driveway, the air and concrete are both 85°F, with 25% relative humidity and near-surface wind of 15 mph. The estimated evaporation is above the specified action level. Which response fits hot-weather practice?

A

Add water at the chute to keep the mix workable, then finish as fast as possible.

B

Begin troweling immediately after screeding so a crust cannot form.

C

Skip curing, because the surface will dry quickly on its own in the wind.

D

Reduce evaporation with a windbreak or shade, dampen the subgrade, use fog spray or an evaporation retardant, place cooler concrete and start curing as soon as finishing ends.

Sections you finish are checked off in the contents.