31.2 Cement, Mix Design & Proportions
Key Takeaways
Current ASTM C150/C150M includes Types I, II, III and V and the IA, IIA and IIIA air-entraining variants. The edition referenced by the 2015 IRC also listed low-heat Type IV.
Compute water-to-cementitious materials ratio by mass and count the free moisture on aggregates as mixing water. Lower w/cm generally increases strength for comparable materials, consolidation and curing.
In Michigan’s severe weathering column, Table R402.2 has distinct 2,500 psi protected, 3,000 psi exposed vertical and 3,500 psi covered exterior flatwork and garage floor rows. Read the applicable air and deicer footnotes.
Absolute volume is mass divided by the product of specific gravity and water density. At 0.50 w/c with 564 lb of cement, target mixing water is 282 lb, or about 34 gallons, before accounting for aggregate surface water.
When using the MRC prescriptive wall limits, check nominal maximum aggregate size against both form width and clearances to reinforcement and forms.
Quick Answer: Start with the required strength, exposure and placement conditions. Balance mixing water, cementitious materials, aggregates and air to fill the target volume. Verify the candidate proportions by trial or qualifying production records.
Portland cement and blended cement designations
To make portland cement, a kiln heats a limestone-based raw mix to form clinker. The clinker is cooled and ground with gypsum or other permitted materials. After mixing with water, the calcium silicates hydrate and form calcium-silicate-hydrate, which binds the aggregate. Tricalcium silicate contributes strongly to early strength, dicalcium silicate contributes more slowly, and the aluminates affect early heat and sulfate performance.
ASTM C150/C150M-24 lists four basic types and the IA, IIA and IIIA air-entraining variants. The 2015 IRC Chapter 44 references the 2012 edition of C150 for the prescriptive concrete-wall provisions, so older Type IV terminology remains relevant to that reference.
| Portland cement designation | Selection |
|---|---|
| Type I | General construction where special cement properties are unnecessary |
| Type II | Moderate sulfate resistance |
| Type III | High early strength, when the schedule or cold-weather plan requires faster strength development |
| Type V | High sulfate resistance, as needed for the specified exposure |
| Type IV, older edition | Low heat of hydration for temperature control in mass concrete |
Type III can help meet an early stripping or loading target. Verify actual in-place strength before either operation. For mass concrete, a specification can require low heat performance, such as Type LH under ASTM C1157, or set a temperature-control requirement for the complete mixture.
ASTM C595 covers blended hydraulic cements such as Type IL portland-limestone, Type IS portland-slag and Type IP portland-pozzolan. Verify the product and any required performance suffix. A Type I/II label represents a dual classification. A different cement is a proposed substitution to be checked against the approved specification.
Supplementary cementitious materials
Supplementary cementitious materials (SCMs) replace part of the portland cement or arrive as part of a blended cement. Choose the type and amount for the actual materials, exposure and placement conditions.
- Fly ash (ASTM C618). Class F fly ash is pozzolanic and can reduce heat and permeability and improve sulfate and alkali-silica resistance, often with slower early strength development. Class C may also have cementitious properties and shows different early-strength and sulfate behavior. Check the proposed combination by testing.
- Slag cement (ASTM C989). This hydraulic material can reduce permeability. Check its rate of strength gain at the expected temperature and verify the blend’s exposure performance.
- Silica fume (ASTM C1240). Its fine particles and pozzolanic reaction can produce high strength and low permeability. Evaluate the water-reducing admixture, finishing and curing needs in the approved mix.
On a cold November placement, ask how the candidate mix develops the strength needed for finishing operations, protection and form removal. Trial or production data for the actual blend and temperatures are a better basis for planning than a fixed delay assigned to all SCMs.
Water, cement and Abrams' law
The water-to-cementitious materials ratio, w/cm, divides effective mixing-water mass by total cementitious material mass. With portland cement as the only binder, this is w/c. With otherwise comparable materials and adequate consolidation and curing, strength generally rises as the ratio falls. Extra water increases the space available for capillary pores. Too little workability can leave voids from poor consolidation, so choose the ratio and placing characteristics together.
| What to check | Why it matters |
|---|---|
| Required strength and production variability | The target average for proportioning can be higher than the specified strength |
| Exposure criteria under the applicable design/specification | The most restrictive governing w/cm limit controls even when strength could be met at a higher ratio |
| Aggregate surface moisture and planned admixtures | These affect actual water content and consistency at placement |
At 564 lb of cement per yd³, adding an unaccounted-for gallon per yd³ increases w/c by about 8.33 ÷ 564 = 0.015. Five extra gallons per yd³ would take a 0.50 mix to about 0.574. For a delivery adjustment, verify the ticket and actual allowance, permitted slump and w/cm before adding any water. Measure and record a permitted addition, remix and retest as required. If there is no water allowance, ask the producer about an authorized water-reducer adjustment or disposition of the load.
Proportioning: absolute volume and trial batch
The absolute-volume method accounts for the volume of each ingredient and the air, totaling 27 ft³ per cubic yard. The trial batch checks the candidate proportions by measuring slump, air, density and yield and testing cylinders at the designated age.
For materials other than air, volume = weight ÷ (specific gravity × 62.4 lb/ft³) using customary units and a consistent aggregate moisture basis. Use the measured specific gravity for each aggregate.
Worked example. Develop a trial batch for a protected footing specified at 3,000 psi. Assume a starting cement content of 564 lb/yd³, w/c of 0.50, 5% design air, cement specific gravity 3.15, and both aggregates at an SSD specific gravity of 2.65. Here the designer allocates the remaining aggregate volume 60% to gravel and 40% to sand.
| Ingredient | Weight per cubic yard | Absolute volume |
|---|---|---|
| Cement | 564 lb | 564 ÷ (3.15 × 62.4) = 2.87 ft³ |
| Mixing water | 282 lb | 282 ÷ 62.4 = 4.52 ft³ |
| Air | Excluded from batch weight | 0.05 × 27 = 1.35 ft³ |
| Gravel, SSD | About 1,812 lb | 0.60 × remaining volume = 10.96 ft³ |
| Sand, SSD | About 1,208 lb | 0.40 × remaining volume = 7.30 ft³ |
| Total | About 3,866 lb | 27.00 ft³ |
The cement and w/c give 282 lb of mixing water, about 33.9 gal/yd³ at 8.33 lb/gal. The theoretical fresh density is 3,866 ÷ 27 ≈ 143 lb/ft³. A 10-yd³ order scales to 5,640 lb of cement and 2,820 lb of mixing water, about 339 gal before adjusting for moisture. Measure actual density and yield and verify the trial strength. The proportions alone cannot establish a 3,000 psi result.
Correct the sand moisture. The 1,208 lb in the table is saturated surface-dry (SSD), with pores filled and the surface free of water. Assume sand absorption of 1%, total moisture of 6%, and gravel at SSD. Both moisture percentages are based on oven-dry mass. Divide 1,208 by 1.01 to get about 1,196 lb oven-dry sand. Batch 1,196 × 1.06 ≈ 1,268 lb of wet sand. The surface water is 1,196 × (0.06 − 0.01) ≈ 59.8 lb, so add 282 − 59.8 ≈ 222.2 lb from the batch water supply. If the correct wet sand is weighed but the full 282 lb of water is added, effective w/c would rise to about 0.606. When aggregate is below SSD, its water demand moves the correction in the opposite direction.
A nominal 1:2:3 volumetric recipe gives proportions by bulk volume. Packing, moisture, water content and materials all affect its yield and strength. Use the approved mix and applicable batching specification. ASTM C685 covers volumetric batching with continuous mixing where that method is allowed.
Aggregates: the skeleton of the mix
Aggregate typically occupies 60 to 75 percent of normal concrete volume. Fine aggregate is mostly sand-size material, while coarse aggregate is predominantly retained on the No. 4 (4.75 mm) sieve. Actual gradations include tolerances and are checked against the applicable ASTM C33 grading limits and project requirements.
- Grading. The size distribution affects voids, paste demand, pumping and finishability. Select a blend that meets the approved mix requirements for both workability and stability.
- Deleterious material. Clay lumps, friable particles, organic impurities and reactive constituents can interfere with strength or durability. Check the ASTM C33 limits and any exposure-specific tests.
- Maximum size. MRC R404.1.3.3.3 and R608.5.1.3 use the lesser of one-fifth the narrowest space between form faces and three-fourths the governing clear distance between bars or between a bar and its form face. If the narrowest form dimension is 6 inches and the tightest clearance is 1 inch, the respective limits are 1.2 inches and 0.75 inch. The smaller controls. The code has an approval exception for removable forms where workability and consolidation prevent voids. Check separate limits under an engineered design, including the applicable slab-depth criterion when using ACI 318.
- Shape and texture. Angular, rough-textured material often needs more water for equal workability than rounded gravel. Confirm the combined effect of grading, paste and admixtures in the trial mix.
Air entrainment and admixtures
Michigan’s amended Table R301.2(1) designates severe weathering. Start with the applicable location and use row in MRC Table R402.2. Its air-entrainment provisions call for total air at 5% to 7% for the specified severe-exposure rows, with the stated garage finish exception. Entrained microscopic air voids relieve pressure as water freezes.
ASTM C494 covers admixtures such as water reducers, retarders and accelerators. ASTM C260 covers air-entraining admixtures. Check chloride limits and project restrictions before specifying an accelerator. Nonchloride products avoid introducing calcium chloride to reinforced work. High-range water reducers can increase flow at the same w/cm when compatible with the rest of the mix.
Minimum strengths under Michigan’s severe-weathering column
| Table R402.2 location or construction | Minimum specified 28-day strength | Total air under the table |
|---|---|---|
| Foundations, basement walls and other concrete protected from weather | 2,500 psi | 5% to 7% if subject to freezing and thawing during construction (note c) |
| Basement and other interior slabs on grade, excluding garage floors | 2,500 psi | Same construction-exposure note |
| Basement, foundation and exterior walls and other vertical concrete exposed to weather | 3,000 psi | 5% to 7% |
| Porches, carport slabs and steps exposed to weather, and garage floors | 3,500 psi | 5% to 7%, subject to the steel-troweled garage-floor option |
| Steel-troweled garage floor using the option in note f | At least 4,000 psi | At least 3% permitted under the option |
Check R402.2 and its footnotes for the cementitious-material limits on the covered deicer-exposed placements. The table leaves other applications, such as a separate driveway, to their applicable specifications. Verify any higher design minimum or other applicable provision, such as the seismic limits for cast-in-place foundation walls or the separate precast foundation provision.
A trial mixture uses 564 lb of cement per cubic yard as its only binder and a water-cement ratio of 0.50. What is the target total mixing water, including free aggregate moisture?
About 17 gallons
About 25 gallons
About 45 gallons
About 34 gallons
Which ASTM C150 portland cement designation is selected when the specification calls for high early strength?
Type III
Type II
Type IV
Type V
What trade-off is commonly considered when selecting Class F fly ash to replace part of the cement in a residential concrete mix?
Faster early strength so forms can routinely be stripped sooner
Less coarse aggregate because Class F fly ash replaces gravel
Potentially lower heat and permeability and better sulfate resistance, with slower early strength development
Built-in air entrainment that removes the need to check total air
Sections you finish are checked off in the contents.