32.3 Concrete Admixtures
Key Takeaways
ASTM C494 classifies chemical admixtures as Type A water-reducing, B retarding, C accelerating, D water-reducing and retarding, E water-reducing and accelerating, F high-range water-reducing, G high-range water-reducing and retarding, and S specific performance.
ASTM C260 covers air-entraining admixtures. MRC Table R402.2 generally uses 5% to 7% total air in the applicable severe-weathering rows. Check construction exposure and the steel-troweled garage floor option separately.
ACI 318 Table 19.3.2.1 gives nonprestressed chloride limits of 1.00%, 0.30% and 0.15% for C0, C1 and C2, respectively, and 0.06% for prestressed concrete. Use the measurement basis and restrictions of the governing edition.
S2 and S3 are sulfate exposure classes. The ACI 318-14 sulfate rows prohibit calcium chloride admixture, and separate provisions address prestressing, aluminum embedments and permanent galvanized forms.
Retarders increase working time, accelerators can shorten set or improve early strength, and water reducers can change flow without added water. Check compatibility, approved dosage and placement conditions.
An admixture is an ingredient added to modify fresh or hardened concrete properties. This section focuses on chemical admixtures. Choose them while the mix is being proportioned and qualify their performance with the actual materials. Use controlled dosing and mixing under the approved procedure.
The ASTM C494 family
ASTM C494 classifies chemical admixtures by their demonstrated function. The test compares the mixture with a control and checks properties relevant to the classification.
| Type | Function | Typical residential use |
|---|---|---|
| A | Water-reducing | Cut water while holding slump; everyday strength and economy |
| B | Retarding | Slow set in hot weather or large pours |
| C | Accelerating | Speed set and early strength in cold weather |
| D | Water-reducing and retarding | Hot-weather walls and large footings |
| E | Water-reducing and accelerating | Cold-weather placement that still needs water reduction |
| F | High-range water-reducing (superplasticizer) | Flowing mixes, ICF walls, congested steel, pumping |
| G | High-range water-reducing and retarding | Flowable mix with extended working time |
| S | Specific performance | Corrosion inhibition, shrinkage reduction and other targeted claims |
At a comparable consistency, a water reducer can achieve the specified slump with less mixing water. At the same cementitious content, this lowers w/cm. In C494 qualification, Types A, D and E use at most 95% of control water, and Types F and G at most 88%. Those correspond to minimum reductions of 5% and 12% in the qualification test. The amount needed for an actual mix comes from trials and the supplier’s data.
Water reducers can also improve flow at the same w/cm. Slump retention depends on product, dose, materials, time and temperature. Use the approved dose and delivery plan. If the concrete needs adjustment at delivery, follow the allowed procedure, remix and retest as required.
Air-entraining admixtures (ASTM C260)
Air-entraining agents promote a system of small, well-distributed voids that relieves pressure from freezing water. The 2015 MRC uses Michigan’s severe column in Table R402.2. Apply 5% to 7% total air to the covered exposed vertical and flatwork applications and to the protected rows when exposed to freezing and thawing during construction. The steel-troweled garage-floor option permits reduction to at least 3% total air with a specified strength of at least 4,000 psi.
For otherwise comparable materials and water content, more air can lower compressive strength. Proportion the mix to meet both specified requirements. Use ASTM C231 when the pressure method suits the aggregate or ASTM C173 for lightweight or porous aggregate. Record results in the testing report and reconcile the report with the delivery ticket.
Retarders and accelerators
Retarders (Type B or D) delay setting, which can extend working time during hot weather or a long placement. Check slump retention and delivery sequencing and plan for consolidation at lift interfaces. A retarder alone cannot ensure a sound joint. A delayed set can extend the window before finishing and protection, especially if the concrete cools.
Accelerators (Type C or E) support earlier setting and/or strength development, depending on the product. Use a suitable approved nonchloride accelerator when needed in steel-reinforced concrete. Continue to meet the specified concrete temperature and cold-weather protection requirements and prepare a thawed, suitable bearing surface.
The chloride problem
Calcium chloride can accelerate setting and early strength, but it also introduces chloride ions. They can destabilize the protective film on embedded steel. Corrosion products take up more space and can crack or spall the surrounding concrete. Count chlorides from all concrete ingredients when evaluating the mix.
Check both the total chloride limit and restrictions on particular admixtures. ACI 318-14 §26.4.1.5.1(c), where applicable through the 2015 MRC, prohibits calcium chloride or chloride-bearing admixtures beyond ingredient impurities in prestressed concrete, concrete with embedded aluminum and concrete cast against permanent galvanized steel forms. Its Table 19.3.2.1 also prohibits calcium chloride admixture in classes S2 and S3, which address sulfates. Moisture and external chlorides belong to the C exposure classes.
| ACI 318-14 corrosion class | In-service exposure | Nonprestressed | Prestressed |
|---|---|---|---|
| C0 | Dry or protected from moisture | 1.00% | 0.06% |
| C1 | Moisture without an external chloride source | 0.30% | 0.06% |
| C2 | Moisture and an external chloride source | 0.15% | 0.06% |
The table values are maximum water-soluble chloride ion as a percent of cement mass under ACI 318-14, with ASTM C1218 testing between 28 and 42 days. Under ACI 318-25 the limits shown use total cementitious mass with a cap on the SCM mass credited, and the code permits calculation from measured ingredient chlorides or C1218 tests. The newer edition also has separate admixture and embedment provisions. Follow the governing edition and any stricter specification. Compare a damp wall without external chlorides (C1) with reinforced concrete in contact with moisture and road deicer (C2) when that exposure classification governs.
Other admixtures worth knowing
- Corrosion inhibitors qualified under ASTM C1582, such as certain calcium nitrite products, can reduce corrosion risk as part of a mixture and cover design.
- Shrinkage reducers can reduce drying shrinkage. Check the Type S performance identified for the specific product and verify compatibility.
- High-range water reducers can help achieve the required flow for placement through dense reinforcement. Check stability, form pressure and applicable consolidation requirements.
- Air-entraining agents use ASTM C260. Confirm air content with the actual mix and handling method.
- Combined admixtures can change rate of set, air content or flow. Evaluate the combination using the specified cementitious materials and temperature range.
Selecting an admixture
| Jobsite condition | Candidate admixture | What to verify |
|---|---|---|
| Hot weather or extended delivery | Type B or D retarder | Placement time, set and finishing under actual temperatures |
| Early strength in cold weather | Approved Type C or E accelerator | Freeze protection, temperature and chloride restrictions |
| Covered freeze-thaw exposure | Air-entraining agent under ASTM C260 | Applicable total-air limit and test method |
| Higher flow at the same w/cm | Type F or G high-range reducer | Stability, flow retention and compatible dosage |
| Chlorides in service | Approved corrosion inhibitor where specified | Mixture limit, cover and exposure design |
| Drying shrinkage of flatwork | Qualified shrinkage reducer | Tested performance and the joint and curing plan |
Field rules
- Verify the submittal. Confirm the admixture, compatible products and dose range.
- Control any adjustment. A permitted addition at delivery, such as an authorized water reducer, requires a measured dose and thorough remixing under the applicable delivery procedure.
- Keep the records. Record adjustments and link the test report to the batch. Review fresh properties after adjustment as required.
- Investigate abnormal behavior. Check time, temperature and proportioning with the producer before deciding the disposition of an off-specification load.
Exam traps
- Type D combines water reduction with retardation. Type E combines water reduction with acceleration.
- Check both the C260 product and the required total air for the application.
- Keep sulfate classes S2 and S3 separate from corrosion classes C0 to C2 and apply the correct ACI edition.
- Follow the approved slump, water and admixture adjustment limits.
Under ASTM C494, a Type D admixture is:
Accelerating
Water-reducing and retarding
High-range water-reducing
Air-entraining
Which admixture is used to help develop early strength for cold-weather steel-reinforced concrete, and what property of the admixture matters to the steel?
Type B retarder, because a faster set reduces chloride corrosion
Air-entraining agent, because lower air content accelerates strength gain
Type C accelerator, with the chloride content and use restrictions checked to protect the steel
Type F superplasticizer, because normal dosing deliberately separates the mix