8.2 Heat Treatment and Hardness Testing

Key Takeaways

  • Material, section and cooling history determine how much martensite forms. A heat treatment label by itself does not establish hardness.

  • Carburizing adds carbon, nitriding adds nitrogen, and induction hardening can transform a selected surface without adding either.

  • Rockwell C uses a diamond cone and 150 kgf total force. The result comes from the permanent depth increase measured at the preliminary force.

  • Hardness results depend on scale, material, surface, thickness and location. A shallow case may require a different scale or a depth profile.

Last updated: November 2026

8.2 Heat Treatment and Hardness Testing

Distinguish phases from the actual treatment result

Heat treatment changes the condition of a material through controlled heating and cooling. In ordinary steels ferrite has a body-centered cubic structure; austenite has a face-centered cubic structure. Pearlite is a layered mixture of ferrite and cementite. When a suitable steel is austenitized and cooled rapidly enough at the location of interest, austenite can transform without diffusion into martensite. Hardness and the martensite fraction depend on the grade, section, achieved heating and cooling. Some austenite or other products may remain. Read the specified process instead of assigning one quench temperature or hardness to every grade.

Annealing and normalizing can prepare stock for an intended level of hardness, machinability or structure. A common full-anneal route for a suitable steel uses slow furnace cooling, while a normalizing route uses air cooling. The schedules and results depend on the grade and section. A hardening route uses the specified heat and quench for that material. Hardenability describes how readily hardness can develop through a section during quenching. It differs from the hardness measured at a particular location. A severe quench can raise the risks of distortion and cracking. Select the medium and cycle from the authorized process.

Tempering reheats hardened steel under controlled conditions to change the hardness and toughness balance and relieve stresses. There can be exceptions to a simple softening trend, including secondary hardening in certain tool steels. Follow the prescribed sequence and timing. Stress-relief treatments can reduce residual stress but can also change material properties depending on the starting condition and cycle. Keep the process specification with the part and leave documented stock for final machining where required.

Distinguish surface treatment mechanisms

ProcessWhat changes the surfaceMachining implication
Carburizing followed by hardeningAdds carbon by diffusion in an appropriate steel before the hardening treatment.A gear may specify effective case depth and surface hardness at named locations. Heavy finish stock removal can consume the required case.
Gas nitridingIntroduces nitrogen; hard nitrides and related surface changes contribute to case properties. It does not require a subsequent hardening quench in the described gas nitriding process.Low distortion is a process advantage. Inspect critical dimensions because changes are still possible.
Induction hardeningHeats a local region electromagnetically and quenches it. It uses the steel's existing composition.The required hard zone may be local, for example at a shaft journal. Check the hardening extent shown on the print.

Suppose a treated shaft needs cleanup after a hardness and case-depth check. The part specification still applies after grinding. If an approved sample shows a 0.030 in effective case measured normal to the old surface and 0.010 in of material is removed from that surface, a simple geometric estimate leaves 0.020 in below the new surface, assuming the profile is unaffected by grinding. Removing 0.010 in from diameter on a cylindrical surface instead removes 0.005 in radially. Use the released process allowance and inspection requirement to confirm the finished condition; heat introduced during grinding may change the result.

Identify what the hardness machine measures

A hardness reading reports response to a specific indentation procedure. Verify the scale, reference block, support, surface preparation, location and minimum thickness. An indentation in a thin part or close to a previous impression or edge can be affected by material outside the intended zone.

  • Rockwell C (HRC) uses a 120° diamond cone with a rounded tip, a 10 kgf preliminary force and a 150 kgf total force. Establish the baseline under the preliminary force, apply the total force under the specified cycle, and return to the preliminary force for the final depth. For the C scale, the conventional number is 100−h/0.002100-h/0.002 with net depth hh in millimeters. A net h=0.080h=0.080 mm gives 60 HRC. Rockwell ball scales use different indenters and force combinations, so always record the scale.
  • Brinell (HBW) uses a tungsten-carbide ball of specified diameter and force; measure the resulting impression diameter using the test procedure. A 10 mm ball with 3000 kgf is one standardized combination, not the only one. A large indent can sample more material but may be unsuitable for a thin or small part. With a 10 mm ball, 3000 kgf and mean impression diameter 4.00 mm, the Brinell equation gives about 229 HBW. Holding ball and force constant, a larger impression gives a lower number.
  • Vickers and Knoop use distinct diamond indenters and optical measurements. A qualified microindentation traverse across a prepared section can assess a hardness gradient. Follow the specified load, spacing and criterion for case depth.

If the drawing calls for 58–62 HRC on a case surface and the shop has one value from a different hardness scale, do not simply compare the numbers. Use the required method or an explicitly authorized, applicable conversion. A surface result alone does not demonstrate the entire case-depth requirement.

SAE heat treatment information, Bodycote hardening, Bodycote gas nitriding, NIST Rockwell guide and NIST hardness methods

Loading diagram...
Heat treatment decisions for a suitable steel
Test Your Knowledge

Which transformation product can form when a suitable steel is austenitized and then cooled quickly enough to suppress diffusional transformation?

A

Coarse pearlite

B

Martensite

C

Solidified graphite

D

A new layer of chromium plating

Test Your Knowledge

Which steel treatment introduces nitrogen at the surface and typically does not require a subsequent hardening quench?

A

Gas carburizing

B

Induction hardening

C

Flame hardening

D

Gas nitriding

Test Your Knowledge

Which force sequence and indenter identify the regular Rockwell C test?

A

Diamond cone, 10 kgf preliminary and 150 kgf total

B

Tungsten-carbide ball, 10 kgf preliminary and 100 kgf total

C

Tungsten-carbide ball, 3000 kgf with optical impression diameter

D

Diamond pyramid, with an optical measurement of the diagonals

Test Your Knowledge

A job requires a surface hardness and an effective case depth. Which plan addresses both requirements?

A

Record only a single core hardness value

B

Infer case depth from the furnace time alone

C

Verify the required surface scale and use the specified depth method, such as a qualified hardness traverse

D

Compare a Brinell value directly with the HRC limits

Sections you finish are checked off in the contents.