7.3 Preheat, Interpass Temperature, Heat Input Calculations & PWHT

Key Takeaways

  • Preheat can reduce cooling rate and the risk of hydrogen cracking in susceptible steels.

  • Use the specified instrument, location and timing for preheat and interpass measurements. Shiny surfaces can make infrared readings unreliable.

  • For steady arc voltage and current, arc energy in kJ/mm is 60VI/(1000S) if travel speed S is in mm/min.

  • Apply the governing measurement method and any specified efficiency factor. Compare results on the same basis and in the same units.

  • Check a post-weld heat-treatment record against the approved cycle, including sensors, ramp rates, soak temperature and hold time.

Last updated: November 2026

Know when temperature is being checked

Preheat brings the joint area to its required temperature before welding. For some steels it slows cooling enough to reduce the likelihood of a hard heat-affected zone (HAZ) and helps diffusible hydrogen escape. Hydrogen cracking risk also depends on material hardenability, weld hydrogen and tensile stress. Thickness, restraint, consumable handling and procedure inputs matter. Obtain the temperature from the issued procedure and material requirements. CWB on preheating and TWI on preventing hydrogen cracking.

Interpass temperature is checked in the weld area before the next pass according to the specified measurement method. The approved procedure may prescribe minimum and maximum values. If a reading is outside either limit, record it and verify the required action before welding continues. Some quenched and tempered steels require particular control of the thermal cycle to achieve the required properties. ISO 13916:2025 measurement scope and TWI on welding quenched and tempered steels.

Take a comparable reading

MethodWhat the reading establishesWhat to verify
Temperature-indicating stickThe contacted surface reached the stick’s rated transition when used correctlyCorrect rating, location and melt indication
Contact probe or thermocoupleSurface temperature at the contact point after the instrument responseEquipment status, contact, location and timing
Infrared thermometerSurface temperature estimated from detected radiationPermitted use, emissivity, reflections and spot size

A polished or freshly ground surface can reflect its surroundings and emit relatively little radiation. An infrared reading can be low or high depending on the setup. Verify an unexpected reading by the specified method. Two readings at different times and locations cannot isolate the error, even when one of the instruments is sensitive to emissivity. Fluke on infrared emissivity and reflected radiation and Markal on temperature-indicating sticks.

Worked temperature check. A job requires at least 120 °C before welding and an interpass range of 120–200 °C, measured by contact at the locations specified in the procedure. The initial reading of 125 °C meets its minimum. Before the cap pass the valid reading is 214 °C, which exceeds the maximum by 14 °C. Record the reading and check that the specified cooling and verification steps are followed before depositing the pass.

Compute energy per unit length

At steady readings of voltage VV in volts and current II in amperes, and forward travel speed SS in millimetres per minute, calculate:

E=60VI1000S.E = \frac{60VI}{1000S}.

Multiplying VIVI by 60 gives joules per minute. Dividing by 1000S1000S converts to kilojoules per millimetre. Using inches per minute yields kilojoules per inch instead. Some welding documents, including the CWB guide for filling out a WPDS, call this quantity heat input. Other documents distinguish arc energy from heat input by multiplying arc energy by a specified efficiency factor kk. Compare like values. For pulsed or waveform-controlled welding, the applicable method may require integrating instantaneous power or using a suitable waveform-capable meter. CWB WPDS preparation guide and TWI on arc welding measurements.

  • At 27 V, 240 A and 300 mm/min, E=388,800/300,000=1.296 kJ/mmE = 388{,}800/300{,}000 = 1.296\,\text{kJ/mm}. If the supplied method specifies k=0.8k=0.8, the resulting heat-input value on that basis is 1.0368 kJ/mm1.0368\,\text{kJ/mm}.
  • A procedure capped at 1.50 kJ/mm1.50\,\text{kJ/mm} on the uncorrected basis is monitored at 26 V, 220 A and 180 mm/min. E=343,200/180,000≈1.91 kJ/mmE=343{,}200/180{,}000 \approx 1.91\,\text{kJ/mm}. Holding voltage and current constant, the speed required to reach the cap mathematically is 228.8 mm/min228.8\,\text{mm/min}. Check all procedure limits before changing any setting. The inspector records the deviation and refers proposed parameter changes to the responsible person.

A stringer progresses with little lateral oscillation. A weave intentionally oscillates across the joint. At the same voltage and current, slower forward travel increases arc energy per unit joint length. Compare actual travel and weave technique with their specified ranges. Weave width alone does not quantify energy.

Read the post-weld heat-treatment record

Post-weld heat treatment (PWHT) is a specified thermal cycle after welding. Subcritical stress-relief treatment can reduce residual stress without going above the lower transformation temperature. Requirements depend on material, thickness, code and application. For a weld that requires PWHT, match the trace or chart to the weld or load, check sensor identification and placement, compare ramp rates and holding temperature and duration with the approved cycle, and record departures. A maximum temperature alone does not show that the required hold or cooling rate was achieved. TWI research on PWHT and residual stress.

Arc energy at 26 V and 220 A (kJ/mm)
Test Your Knowledge

A steady GMAW pass runs at 28 V, 250 A and 280 mm/min. What is the arc energy per unit length before applying any efficiency factor?

A

0.75 kJ/mm

B

1.50 kJ/mm

C

2.10 kJ/mm

D

2.80 kJ/mm

Test Your Knowledge

A high-emissivity IR setting is used to read 85 °C on a shiny bevel. The procedure requires a contact measurement at a defined location and time. What should the inspector do?

A

Follow the specified contact method and verify that reading against the procedure.

B

Accept the IR reading as the temperature of every part of the joint.

C

Increase the IR setting until it shows the required number.

D

Apply the same fixed temperature correction on all shiny metals.

Test Your Knowledge

A steel weld requires subcritical stress-relief PWHT. Which record supports a check of the cycle?

A

The next welder’s preheat log.

B

A single reading at the peak temperature.

C

A trace with time and temperature, connected to the weld and the specified sensors, that can be checked for ramp rates, holding temperature and duration.

D

Only the date the furnace was started.