6.4 Gas Tungsten Arc Welding (GTAW), Stud Welding & ESW/EGW Awareness
Key Takeaways
Gas tungsten arc welding uses a nonconsumable tungsten electrode, shielding gas and optional separately added filler.
DCEN is common for steel GTAW. In AC aluminium GTAW the electrode-positive portion contributes oxide cleaning.
Verify the specified shielding and root protection. Tungsten contact with the pool can contaminate the electrode or weld.
Drawn-arc stud welding lifts the stud to form an arc and plunges it into the pool. Inspect using the applicable stud requirements.
Electroslag welding uses resistance heating after startup. Electrogas welding maintains an arc.
Recognize gas tungsten arc welding
Gas tungsten arc welding (GTAW), often called TIG, forms an arc between a nonconsumable tungsten electrode and the workpiece. Inert gas protects the arc and pool. Filler can be fed separately or the approved weld can be made without filler. A commonly used power source is constant current. From an inspection perspective, the separate electrode and filler controls make it important to identify both. AWS overview of GTAW.
Compare DC electrode negative and AC
Many steel and stainless GTAW procedures specify direct current electrode negative (DCEN). Many aluminium GTAW procedures specify alternating current (AC). During the electrode-positive portion of an AC cycle, the work acts as the cathode and the process can disrupt its surface oxide. During the electrode-negative portion, the arc is directed toward producing penetration into the work with reduced heating of the tungsten compared with electrode positive. AC balance and starting method depend on the power source and procedure.
Check the approved settings even if a different setup could weld the same material. AC cleaning does not replace joint preparation. A drawing that calls for clean, prepared aluminium still requires verification before welding. Miller Electric on GTAW AC balance.
Track shielding and electrode condition
Record the specified torch gas, its actual delivery and conditions around the weld. For some open-root stainless or reactive alloy applications, the procedure requires protective gas on the back of the joint. An acceptable torch flow gives no direct evidence about coverage on the reverse side. Look for the assigned purge verification and evaluate root oxidation against the procedure and product requirements.
Tungsten contacting the pool can contaminate the electrode tip and can leave tungsten in the weld. A contaminated tip can affect arc behaviour. Record what was observed and verify the approved corrective step. In a conventional film radiograph a dense tungsten inclusion can appear lighter than the surrounding weld metal. A qualified radiographer assesses the image and its interpretation. The surface appearance alone cannot establish whether a tungsten particle remains inside. CWB radiography explanation.
Follow a drawn-arc stud welding cycle
A drawn-arc stud weld joins a stud end to a base surface. In a typical ceramic ferrule setup, the gun holds the stud against the base material. At the start it lifts the stud, and the arc melts the end of the stud and adjacent base material. The tool plunges the stud into the molten pool. The ferrule helps contain the pool and form the flash around the base. Where a ferrule is used, remove it after the prescribed cooling so the area can be inspected.
For work under CSA W59, CWB identifies a qualification program for stud bases. Verify that the required stud is qualified and traceable, and check the applicable installation procedure and test plan. Product qualification and the inspections of actual production welds are separate checks. CWB stud base qualification and Nelson stud equipment manual.
Worked inspection. Several ferrules remain in place and one exposed stud has missing flash over part of its base. Identify the affected studs and obtain the required access for visual inspection. Record the observed flash and compare the height, position and other requirements with the project criteria. Use the stated procedure for any required mechanical test or replacement. A bend angle learned for a different code or test stage cannot determine what to do here.
Distinguish electroslag and electrogas
Electroslag welding (ESW) can join a vertical joint using a pool contained by shoes or backing. An arc starts the process and melts flux. After the conductive slag forms, the arc stops and resistance heating through the molten slag supplies heat while welding progresses.
Electrogas welding (EGW) also uses a contained vertical pool, but the electric arc continues to supply heat. Depending on the process variant and electrode, external shielding gas may or may not be used. Both processes can weld a joint in a single progressive pass when their procedure permits it. Their electrical and thermal conditions can affect the weld and heat-affected zone. Confirm the specification permits the selected process and identifies the required procedure and examination. AWS electroslag process workbook and AWS recommended practices for electrogas welding.
Recognize welding without an arc
In resistance spot welding, electrodes press overlapping sheets together and conduct current through them. Electrical resistance produces heat, and a local weld nugget forms at the interface. A surface indentation can help locate a spot but cannot establish nugget size. Use the specified test and record the result against that weld or sample. TWI on resistance spot welding.
In oxyfuel welding, the oxygen and fuel gas flame provides the heat to melt the joint edges. In conventional oxyfuel cutting of steel the flame preheats the metal and an oxygen jet drives oxidation and clears the cut. Friction welding uses mechanical motion and force to generate heat and join in the solid state. Each process has its own procedure and inspection requirements. TWI on oxyfuel welding and TWI on friction welding.
Why does a procedure specify alternating current for a typical aluminium GTAW application?
To eliminate shielding gas.
To keep the workpiece cold.
Electrode positive contributes oxide cleaning, and electrode negative supports penetration.
Aluminium cannot conduct direct current.
Several stud ferrules remain in place and an exposed stud has incomplete flash. Which response fits the inspection assignment?
Accept all studs by estimated perimeter coverage.
Keep the ferrules on and accept the visible height alone.
Cut out every stud before checking requirements.
Expose the weld bases for inspection, record the apparent deficiency and follow the applicable criteria and test or repair procedure.
Which statement distinguishes electroslag welding from electrogas welding?
After startup, ESW uses resistance heating in molten slag. EGW uses a continuing electric arc.
ESW uses a torch flame and EGW uses mechanical pressure.
Both processes obtain all heat from resistance through a solid electrode.
EGW always uses a nonconsumable tungsten electrode.
Match each welding process with how it generates heat.
Match each item on the left with the correct item on the right
Resistance spot welding
Oxyfuel welding
Friction welding
Sections you finish are checked off in the contents.