12.2 Surface & Dimensional Faults: Undercut, Overlap, Reinforcement & Fit-Up (WFIC-301)
Key Takeaways
A discontinuity is an observed interruption or irregularity. A defect fails an applicable requirement.
Undercut removes material at a toe or root. Overlap is deposited metal projecting without fusion.
Use the specified reference surface and limits for weld profile and preparation measurements.
Check both dimensions and observable indications. Route decisions and repairs through the approved procedure.
Describe before deciding
An indication is something seen or detected that needs interpretation. A discontinuity is an interruption in the normal structure or geometry. A discontinuity is a defect when it makes the weld or component unacceptable under the applicable criteria. Record what is visible and where it occurs. Compare it to the stated requirements for that weld, edition and loading condition. Similar-looking indications can have different causes. CWB on weld defects and their significance and ISO 6520-1 description and classification scope.
Distinguish toe and face conditions
| Condition | What to look for and record |
|---|---|
| Undercut | An unfilled groove melted into parent metal near a weld toe or root. Check depth from the appropriate reference, extent and location |
| Overlap | Weld metal projecting past the toe or root onto a surface with no fusion there. Record the affected edge and length. Compare with the exact criterion |
| Reinforcement | Weld metal above the adjacent reference surface of a groove weld. Measure the required face or root height. Apply the specified limit |
| Convexity and concavity | Outward bulge or inward profile relative to the chord between fillet toes. Use a suitable gauge for the characteristic required |
| Underfill and root concavity | A low groove-weld surface, or a depressed root profile in the appropriate location. Compare with the drawing or code and the correct reference surface |
A steep weld toe or sharp undercut can concentrate stress. A large crown does not establish adequate fusion or code compliance. On a concave fillet, inspect the feature that the stated leg, profile or throat criterion actually requires. Welding current, speed, arc length, gun angle and contamination can affect profile. Treat them as investigation leads unless there is evidence for a specific cause. TWI on weld shape and causes and Gal Gage weld profile directions.
Compare visible dimensions
Linear misalignment, sometimes called hi-lo, is offset across joint members, such as an internal step between pipe walls. Document the surfaces used, the location and the magnitude. Excess offset can affect joint behaviour and welding access. Check the actual joint preparation, including root opening, land and bevel, against the specified drawing and procedure. Other material indications can appear at a prepared edge. A line parallel to a rolled plate face could be a lamination. Record location and extent and refer for the specified investigation. A suspected lamination differs from a weld toe crack or from lamellar tearing due to through-thickness strain. TWI on material selection and laminations and TWI on lamellar tearing.
Worked geometry. In a flat-faced ideal 90° fillet the theoretical geometric throat is the altitude to the face. For two 8 mm legs it is , rounded. For a flat face between 8 mm and 5 mm legs it is . The smaller ideal throat illustrates why recording both legs matters. A visible concave face can lie closer to the root than the line joining the toes. Use the applicable profile or size requirement and measurement method. The illustrated geometry alone does not establish an allowable load, internal fusion or the actual code acceptance. CWB on fillet geometry.
Report material or weld surface anomalies
Spatter consists of expelled metal droplets that stick near the weld. In addition to any appearance requirements, heavy spatter can obstruct examination or other operations. Check whether the surface is suitable for the specified inspection. An arc strike on adjacent parent metal can cause local melting, hardness and cracking in susceptible materials. Record its location and use the governing disposition and any required additional examination. Do not authorize grinding or welding without an applicable procedure and disposition. CWB on welding defects and TWI on steel microstructure and cooling rate.
Worked practical sample. Under the CWB GWS 2026-R7, a weld sample’s two fillet legs measure 8 mm and 5 mm. Clause 3.1(k) limits the difference between unequal legs to 2 mm. Here the leg difference is 3 mm, which exceeds that criterion by 1 mm. If a separate sample’s joint offset is 1.5 mm, compare that with the 1 mm joint-offset requirement in clause 3.2(e). The limits apply to those practical exam samples. CWB practical GWS.
A root opening example uses the same difference between measurement and disposition. If a drawing calls for a 3 mm root opening on a GWS sample, clause 3.2(f) allows 2–4 mm. A value of 4.0 mm is inside that range and 4.5 mm exceeds it. Make sure the observation describes the opening. A step between the joint members is measured and assessed separately.
Metal protrudes beyond a weld toe onto the plate surface without fusion under the protrusion. Which condition describes it?
Undercut
Overlap
A specified flush finish
Linear misalignment
An apparent arc strike lies on plate away from the joint. Which three actions fit the inspection before disposition?
Select all that apply
Record the location and visible features.
Ignore it because it lies outside the weld face.
Identify the applicable criterion and report it to the responsible person.
Preserve the traceable record and verify any actions required by the approved disposition.
On a CWB practical sample the two legs measure 8 mm and 5 mm. How do they compare with GWS 2026-R7 clause 3.1(k)?
They meet the criterion because the sum is 13 mm.
They meet the criterion because one leg is 8 mm.
The applicable difference is 1 mm, below the limit.
The difference is 3 mm, which exceeds the 2 mm limit.