8.4 Mechanical, Chemical & Metallographic Examinations
Key Takeaways
Select a test for the property or indication being evaluated, and check the specified method and specimen location.
Tension, guided bend, impact and hardness tests establish different properties or responses.
Use a validated chemistry method for the element and alloy. Handheld XRF cannot directly verify carbon.
Macro and micro sections reveal different features. Report the location and orientation of the section.
Start with the required evidence
The drawing, procedure qualification requirements, test plan or applicable code specifies which properties or discontinuities to evaluate. A satisfactory bend does not establish the impact energy. A correct material chemistry does not establish weld fusion. Check what the test measures, where the specimen came from and which criterion applies to that result. CWB gives examples of mechanical testing for procedure and personnel qualification. Use the applicable evaluation instructions and the designated laboratory process. CWB options for evaluating test plates.
Mechanical testing
| Test | What is measured or observed | What the reviewer verifies |
|---|---|---|
| Transverse tension | A specimen across a butt weld is loaded in tension to determine tensile strength and location of fracture | Specimen orientation, original area, maximum force, calculated stress and fracture location |
| Guided bend | A specimen is bent to expose relevant openings on the tension surface under prescribed deformation | Face, root or side bend specified, specimen identity, bend and examined surface, applicable limits |
| Charpy impact | A pendulum breaks a notched specimen and the absorbed energy is recorded | Test temperature, notch orientation and location, energy in joules and any individual and average limits |
| Indentation hardness | A specified indentation test quantifies resistance to indentation at selected locations | Test method, scale or load and exact locations in the weld, HAZ or base metal |
A face-bend specimen places the weld face on the outer, tensile surface. A root bend places the root there. A side bend places a prepared transverse side of the weld on the tensile surface. Use the result for its intended qualification assessment. For impact work, a result from the weld centreline and one from a specified HAZ location answer different questions. The temperature and specimen dimensions also matter. ISO weld tension, bend, Charpy energy, impact specimen location and orientation and hardness.
Worked result. A transverse tension specimen has an original cross-sectional area of 120 mm². The maximum load is 58.8 kN. Tensile strength is , or 490 MPa. If the example calls for a minimum of 480 MPa, the strength result exceeds it by 10 MPa. Record the actual fracture location and check the other required acceptance provisions before making a qualification decision.
Chemical analysis and alloy identification
A lab may confirm chemical composition against a material specification or resolve an identification problem. The test method has to measure the required element in the relevant alloy and range. For example, an applicable spark atomic emission method can analyze carbon and low-alloy steel. An appropriate combustion method can determine carbon in steels within its scope. Handheld X-ray fluorescence (XRF) is useful for alloy screening, including identifying some stainless families, but it cannot directly measure carbon. Similar readings for chromium and nickel therefore cannot establish that stainless stock meets a low-carbon grade limit. ASTM on spark spectrometry, ASTM on combustion and fusion methods and Evident on XRF alloy identification.
For example, two physically similar steel pieces have lost their markings. Record the IDs and isolate the pieces under the project process. Commission the specified analysis if authorized. The results show which chemistry was measured on which piece. Restoring acceptance may also require a traceable link to the material report and the required mechanical properties.
Macroscopic and microscopic examination
A laboratory can cut a section at a documented location, prepare its surface and etch as required to show the weld and surrounding metal. Macroscopic examination shows features such as weld profile, penetration and the visible fusion pattern at that section. Microscopic examination uses a prepared specimen and higher magnification to assess features such as grain structure, phases or small discontinuities. A polished cross-section may be used before or after etching as the method requires. A section is evidence at the sampled plane. If the question is whether a condition extends along the entire weld, obtain the additional examination called for by the test plan. ISO macroscopic and microscopic weld examination.
Before reading any result, confirm the coupon or piece ID, the specimen cut location and orientation, the method, the units and the acceptance basis. Link the lab report to the weld or material record. Escalate missing identifiers or results with the responsible supervisor before the test is accepted.
A transverse tensile specimen carries a maximum load of 58.8 kN and has an original area of 120 mm². What is its calculated tensile strength?
49 MPa
480 MPa
490 MPa
7056 MPa
A handheld XRF result identifies a stainless alloy family. The requirement is to verify that the piece meets the specified maximum carbon content. What should the inspector obtain?
A second XRF reading of the chromium concentration.
An applicable, validated analysis that measures carbon on the traceable piece.
A Charpy impact result for a coupon from the same specification.
A face bend across the weld on the stock.
Match each examination with the evidence it provides.
Match each item on the left with the correct item on the right
Charpy impact
Guided bend
Macrosection
Microscopic section
Sections you finish are checked off in the contents.