4.2 Oxyfuel Cutting Techniques

Key Takeaways

  • Use the chart for the actual torch, fuel, tip and thickness. Verify standoff and oxygen delivery for the operation.

  • Use the specified method for straight cutting, piercing, beveling, washing and gouging. Control the path of slag and support the drop piece.

  • Check cut geometry, slag and drag lines. Verify the approved bevel angle and root face before fit-up.

  • Select a mechanical method when the material, tolerances or work controls rule out oxyfuel. Verify ignition and line-opening hazards for the chosen method.

  • Identify and isolate a used line, control residual contents and verify the required atmosphere, authorization and fire watch before applying heat.

Last updated: November 2026

Oxyfuel Cutting Techniques

Quick Answer: Choose the tip and delivery pressures from the manufacturer’s chart. Use an edge start for a straight cut when the job permits it, and use the prescribed piercing procedure for an internal start. Check bevel angle, root face, cut quality and remaining wall before accepting a weld preparation. Select a mechanical method when thermal cutting conflicts with the material, design or work controls.

Tip selection and standoff distance

Choose a chart for the torch, fuel, tip series, material thickness and operation. Use the required preheat and cutting oxygen ranges for the actual configuration. A mis-sized tip can give an uneven cut even when the regulator gauge seems normal.

Reading a chart. The Victor Type 101 table lists a size 1 tip (0330-0005) at ¾ in. material thickness. The row distinguishes 3–5 psig acetylene from 30–35 psig cutting oxygen and 4–7 psig preheat oxygen. These are the published values for that row. Apply the chart and manual for the actual torch and gas paths. Some hand torches adjust preheat flow at the attachment instead of having a separate preheat oxygen regulator. Recheck oxygen delivery under flow.

Standoff is the distance from the tip to the work. Use the distance and cutting angle specified for the nozzle, fuel and cut. For a square cut, align the jet normal to the surface at the point of cutting. Watch the cut as well as the torch position.

ErrorPossible result
Tip contacts work or slag reaches the tipFouled or overheated tip, abnormal flame and poor start
Tip too far from workSpread preheat, disturbed jet and an uneven top edge
Torch tilted during a square cutCut face angled across the wall
Travel too fastHeavy drag, lower-edge slag or incomplete severance
Travel too slowLocally overheated edge, excess slag or a kerf that closes up

Straight-line cutting

Use this sequence for an edge start on plate. On pipe, support and position the work for the planned torch path.

  1. Mark the cut line with a suitable layout tool. Secure the work and support the drop piece before starting. Clear people, hoses and combustibles from the sparks and slag path.
  2. Preheat the edge or start point to kindling temperature.
  3. Apply the cutting oxygen as directed. Once the jet penetrates, advance steadily so the cut stays through the thickness.
  4. Complete the cut under control and confirm that the offcut is stable before handling it.

On pipe, common methods include:

  • Freehand with wrap-around layout
  • Pipe beveling / cutting machines (oxyfuel or plasma)
  • Rollers or positioners that rotate the pipe under a fixed torch

For butt-weld ends, a square cut is only the first step—bevel geometry is next.

Piercing

Piercing starts in solid material away from an edge. Check that the tip and procedure permit piercing that thickness. Start on the scrap side of the finished line when the layout allows, so the irregular start does not damage the finished edge. Keep people out of the upper and lower spatter paths and clear the space beneath the work.

Preheat to kindling temperature. In the Victor hand-torch example, tilt the tip slightly to direct spatter safely away as you start the pierce. Once the hole is through, return to the planned cutting angle and standoff and advance. Thicker material or machine cutting may require a different pierce sequence. An oxyfuel opening in existing process pipe requires the approved line-isolation and hot-work procedure. Section 13.1 covers the separately engineered process for a live-line hot tap.

Bevels for weld preparation

Use the issued joint detail and WPS. In the Section 6.1 single-V example, two 37.5° bevels give a 75° included groove angle. The example specifies a nominal 1/16 in. root face. Other joints or materials may use a different preparation. Oxyfuel can cut bevels by:

  • Tilting a hand torch to the specified angle
  • Using a beveling attachment or track torch
  • Machine cutting with a bevel head

After thermal beveling:

  • Remove slag and verify a reasonably smooth, true face as required by ASME B31.3-2024 §328.4.2 for the process-piping example. Follow any specified cleaning or finishing requirements.
  • Verify the root face and bevel angle with a gauge.
  • Check that corrective trimming, when permitted, preserves the required wall. Hold deep notches or damage for the approved disposition.

Key Point: Assessment items often link cutting quality to weld prep. A cut that is “through” but not to drawing geometry still fails the job.

Washing and gouging

OperationPurposeTorch action (concept)
WashingRemove nuts, lugs, temporary attachments, or excess metal from a surface with a sweeping oxygen washPreheat then use cutting oxygen in a sweeping motion to wash metal away without necessarily severing a full thickness like a kerf cut
GougingCut a groove to remove weld metal, cracks, or to back-gouge a jointSpecialized gouging tips / technique produce a controlled groove rather than a through-kerf

On pipe, use these methods only when the procedure permits thermal metal removal. A Victor Type 118 tip is designed for operations including gouging and rivet washing. When removing a defect or attachment, inspect the exposed base metal and verify the required remaining wall before release. If its condition or thickness falls below the approved requirement, hold it for disposition. Extra grinding can make the loss worse.

Reading cut quality and common defects

ObservationLikely causeCorrection direction
Drag lines lag heavily / cut fails throughTravel too fast, tip too small, O₂ pressure low, dirty tipSlow down, correct tip/pressure, clean tip
Top edge melted / roundedTravel too slow, tip too large, standoff wrongSpeed up, right tip, correct distance
Slag stuck hard on bottomSpeed/pressure/tip mismatch; dirty plateAdjust parameters; clean plate; deslag properly
Uneven bevel / wandering kerfUnsteady hands, no guide, wrong angleUse guide/track; practice body position
Irregular kerf / notchesUnsteady travel, popping, contaminated surfaceClean metal; stable motion; check tip
Abnormal pop, persistent hiss or possible flame travel into a hoseA transient backfire, sustained internal burning or flashback, depending on the evidenceStop and apply the model’s abnormal-flame procedure in Section 4.1. Keep flashback-exposed equipment out of service for assessment.

Drag lines show the path of the cutting reaction through the thickness. Pronounced lag accompanied by incomplete severance suggests that the cut is falling behind the torch. Check the chart, jet and tip condition, then correct the travel speed. Judge the cut against its required geometry and finish.

When mechanical cutting is preferred

Choose saws, abrasive cut-off, band saws, lathes, cold cutters, or milling when:

  • Specs limit heat-affected zone or forbid thermal cutting on that alloy/service
  • You need high dimensional accuracy without heavy grind cleanup
  • Coatings, insulation, or nearby equipment cannot tolerate slag and sparks
  • Conventional oxyfuel cutting is unsuitable for the material, as with many stainless steels and nonferrous metals
  • Shop production favors repeatable machine cycles over freehand torch work

Choose the mechanical tool for the material, atmosphere and task. Abrasive wheels can create sparks. Follow the line-opening controls when contents or isolation are uncertain even if the proposed method uses no torch.

Safety around used pipe and residual contents

The CSB Sunoco investigation documents a flash fire during hot work on piping that contained residual crude oil. A cool pipe or a drained low point alone does not establish that the full cut zone is safe.

  1. Identify the line, its service history and the limits of the job on the drawings and in the field.
  2. Follow the line-opening procedure. Isolate and verify zero hazardous energy before disturbing the boundary. Establish and verify any required positive isolation through the prescribed first-break controls (Section 1.4).
  3. Drain, clean, and purge or ventilate according to the authorized procedure. Check low points, dead legs and adjacent connected spaces. Establish the atmosphere and monitoring requirements before heating. Never use oxygen to purge.
  4. Obtain the applicable hot-work authorization and fire watch before cutting. Follow the project’s controls for oily or coated workpieces, slag, fumes and changing atmospheric conditions. Federal construction §1926.352 and covered general-industry §§1910.252 and 1910.119(k) apply in their respective settings.

Stop and resolve uncertain contents, isolation or atmosphere before proceeding. Cutting or heating can ignite residues or release vapors even when the outside of the pipe looks clean.

Scenario: beveling a 6-inch carbon spool

The approved drawing specifies the single-V preparation described in Section 6.1. A freehand bevel leaves patches of slag and the root face varies from almost zero to 3/16 in. Remove the slag to inspect the profile. Check the remaining length and wall before re-cutting with a guide or machining to the specified angle and land. If the spool cannot meet the dimensions, hold it for disposition. Recheck the fit and WPS before tacking.

Putting cutting techniques together

  1. Choose the tip and gas delivery settings for the task. Confirm delivery settings with the gas flowing as directed. Inspect the resulting cut.
  2. Control standoff, angle and travel. Use the prescribed edge-start or piercing technique.
  3. Use the approved procedure for washing, gouging and correction. Check the remaining metal, cut geometry and finish.
  4. Review the material and work environment before choosing thermal or mechanical cutting.
  5. Resolve residual contents, energy isolation and hot-work controls before cutting used piping.
Test Your Knowledge

What is the most appropriate primary reference for selecting an oxyfuel cutting tip size and approximate working pressures?

A

Whatever pressures were left on the regulators from the previous shift

B

The largest tip available to finish faster

C

The manufacturer tip chart matched to material thickness (and fuel type)

D

A single universal tip number used for all pipe walls

Test Your Knowledge

In the Victor hand-torch example, why does the operator tilt the tip slightly at the start of a pierce?

A

To direct sparks and molten slag safely away from the tip and operator

B

To operate acetylene above its delivery pressure limit

C

To change the preheat from neutral to carburizing

D

To eliminate the need for eye and face protection

Test Your Knowledge

A cut face shows extremely lagged drag lines and the piece did not sever cleanly. Which adjustment is the best first troubleshooting direction?

A

Travel faster and raise oxygen pressure without limit

B

Switch immediately to a carburizing flame with a long feather

C

Remove flashback arrestors to increase gas flow

D

Verify tip and oxygen delivery against the chart and correct the travel rate if the cut is falling behind

Test Your Knowledge

A pipefitter must open a process line that previously carried flammable liquid. Residues may remain. What is the correct approach before oxyfuel cutting?

A

Cut immediately if the line feels cool to the touch

B

Verify isolation and control residues, confirm the required atmosphere and obtain the applicable authorization before applying heat

C

Crack a drain valve and light the torch to burn the inside clean

D

Use oxygen to purge the line before heating

Sections you finish are checked off in the contents.